bob you should take up tiling mate !Would not use the stain stop on terracotta, discussion with Marc , was for a external terrace.
Lithofin modern method is for internal, and a nice light finish ,rather than a darker oil and wax. The ease of water based products and mostly the ease in which the client will maintain and top up the floor after you have installed. Used tons of this stuff restoration wise as clients wanted an easy to look after floor.
Generally, lay the tiles , leave to dry until all moisture released( 7-10 days for me, or until fully dry, yes I'm obsessed with drying times)
Saturate 1-2 coats of the impregnator before leaving overnight to cure.
Point in the terracotta , ideal not slurry ,unless a very closed pore- check grout release on two unlaid tiles you can impregnate- for testing
Once this grouting/ pointing is fully dry , depending on depth and width
Re impregnate one coat of the terracotta impreg.
After this has dried, sponge on 2-4 neat coats (maybe more if a really ruff hand made) of the terracotta sealant with a jumbo car sponge, dries in 40 min -1 hour so you will get these on in one day.
No buffing , self sheening
Clients maintain with easy care , and top up when required.
They can use 1/4 bucket of clean water, add a mug of the sealant, mop through leaving a slight wet look, leave to dry - job done , nice and easy.
This Has one over coat in 12 years. Must admit its not a high foot traffic area. But is still used daily.